How to Prepare Oil-soluble Tungsten Disulfide Nanosheet?

How to prepare oil-soluble tungsten disulfide nanosheet? The researchers used tungsten hexachloride as the source of tungsten, and thioacetamide and thiourea as the active sulfur sources, and reacted at a constant temperature of 100-200 °C for 60 min in the presence of surface modifiers to obtain oil-soluble WS2 nanosheets. The obtained oil-soluble WS2 nanosheets have high purity, uniform size and two-dimensional sheet structure, and have broad application prospects in the fields of lubricant nano additives and the like.

More details, please visit:
http://tungsten-disulfide.com/index.html

how to prepare oil-soluble tungsten disulfide nanosheet? picture

Preparation of Oil-soluble Tungsten Disulfide Nanosheet
Add 3.9656 g tungsten hexachloride, 20 g oleylamine and 10 g octadecene in a 500 mL flask, heat the above mixture to 140 °C, keep at constant temperature for 10 min, add 5 g of oleylamine solution containing 1.5026 g of thioacetamide, and warm up to 200 °C, constant temperature reacted for 3 h, and then the product was centrifugally washed with ethanol to obtain a black semi-solid oil-soluble tungsten disulfide nanosheets.

Comments are closed.

Address: 3F, No.25-1 WH Rd., Xiamen Software Park Ⅱ, FJ 361008,China Copyright ? 1997 - 2025 CTIA All Rights Reserved
Phone:+86-592-5129696,+86-592-5129595;    Email: sales@chinatungsten.com
舊版